CCS DH500 (also written CCS D500, CCS/D500, CCS Grade D500 or DH500 steel plate) is a high-strength steel for welded marine and offshore structures certified by the China Classification Society (CCS) to CCS Rules for Materials and Welding (2024), Part 1, Chapter 3, Section 4 (High Strength Steels for Welded Structures). The number 500 is the minimum yield strength in MPa (up to 50 mm), tensile strength is 590–770 MPa, and the letter D sets the Charpy V-notch test temperature of −20°C. It is delivered thermo-mechanically rolled (TM) or quenched and tempered (QT) and corresponds to grade DH500 in IACS UR W16.

Gangsteel, a steel plate exporter, supplies CCS DH500 plate with CCS class certificates; the requirements below are taken directly from the current CCS rules.

Related CCS grades: CCS AH500 steel plate, CCS EH500 steel plate, CCS FH500 steel plate, CCS DH460 steel plate, CCS DH550 steel plate.

CCS DH500 chemical composition

CCS DH500 chemical composition, heat (ladle) analysis, % max unless stated, by delivery condition
ElementHeat analysis, TMHeat analysis, QT
C≤ 0.16≤ 0.18
Mn1.00–1.70≤ 1.70
Si≤ 0.60≤ 0.80
P≤ 0.025≤ 0.025
S≤ 0.015≤ 0.015
Al (total)≥ 0.02≥ 0.018
Nb≤ 0.05≤ 0.06
V≤ 0.12≤ 0.12
Ti≤ 0.05≤ 0.05
Ni≤ 2.00≤ 2.00
Cu≤ 0.55≤ 0.50
Cr≤ 0.50≤ 1.50
Mo≤ 0.50≤ 0.70
N≤ 0.025≤ 0.015

 

Source: CCS Rules for Materials and Welding (2024), Part 1, Chapter 3, Table 3.4.3.2 (same values as IACS UR W16 Rev.3). Notes: Nb+V+Ti ≤ 0.26% and Mo+Cr ≤ 0.65% (not applicable to QT); total Al/N ≥ 2:1 unless other nitrogen-binding elements are used; Ni above 2.00% may be approved by CCS; boron, if added, ≤ 0.005%. CCS specifies the chemical composition as a heat (ladle) analysis only; the Rules give no product (check) analysis tolerances for these plates, so no product-analysis column is shown. If a product analysis is required, agree the tolerances in the order.

CCS DH500 mechanical properties and impact test

CCS DH500 tensile and Charpy V-notch requirements
Thickness (mm)Yield ReH min (MPa)Tensile Rm (MPa)
3 ≤ t ≤ 50500590–770
50 < t ≤ 100480590–770
100 < t ≤ 250440540–720
CCS DH500 elongation and impact energy
Elongation A5 min, T (%)Elongation A5 min, L (%)Charpy test temp.KV avg min, T (J)KV avg min, L (J)
1719−20°C3350

Source: CCS Rules for Materials and Welding (2024), Part 1, Chapter 3, Table 3.4.7.4. Plates over 600 mm wide are impact tested transversely (T value applies). For N/NR and TM plates one impact test is taken from each piece; for QT plates from each individually heat-treated piece. Above 50 mm, impact specimens are taken at t/4 and t/2.

CCS DH500 maximum carbon equivalent (plates)
Delivery conditionCeq t ≤ 50 mmCeq 50 < t ≤ 100 mmCeq 100 < t ≤ 250 mmCETPcm
TM0.460.480.500.320.24
QT0.480.500.540.340.25

Table 3.4.3.4. Ceq = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15; CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40 (H460 and above, at the mill’s option); Pcm may be used for TM and QT steels with C ≤ 0.12%. n/a = not applicable.

CCS DH500 thickness range and delivery condition

CCS DH500 maximum plate thickness by delivery condition
Delivery conditionMax plate thickness (mm)
TM150
QT150

Table 3.4.6.2. Thicker plates (N over 250 mm, QT over 150 mm) need special consideration by CCS. Yield and tensile requirements fall in steps above 50 mm and 100 mm, as shown in the table above.

CCS DH500 equivalent grades

CCS DH500 equivalent grades of other classification societies
Standard / societyEquivalent grade
IACS UR W16DH500
ABSAB/DQ51
DNVVL D500
LRLR DH50
ASTM A131no equivalent (A131 stops at the 40 strength level)

The IACS member societies use the same unified requirements, so these grades match in chemistry and properties. A plate still needs the certificate of the vessel’s own class society; one plate can carry dual or multiple class certification only when each society’s surveyor witnesses the tests.

CCS DH500 FAQ

Is CCS D500 the same as CCS DH500?

Yes. CCS lists the grade as DH500; D500 is a common shorthand for the same steel.

What is the yield strength of CCS DH500?

Minimum 500 MPa up to 50 mm, 480 MPa for 50–100 mm and 440 MPa for 100–250 mm. Tensile strength is 590–770 MPa (up to 100 mm).

What is the impact test temperature of CCS DH500?

−20°C, with a minimum average of 33 J transverse or 50 J longitudinal.

What is CCS DH500 equivalent to?

DH500 in IACS UR W16, ABS AB/DQ51, DNV VL D500 and LR DH50. ASTM A131 has no grade at this strength.

How is CCS DH500 supplied?

TM (including TM with accelerated cooling or direct quenching and tempering) or QT. The chemistry and carbon-equivalent limits depend on the delivery condition.

What is the maximum thickness of CCS DH500 plate?

Up to 150 mm in TM or QT condition; thicker plates need special consideration by CCS.

What is the CEV of CCS DH500?

Ceq maximum for plates up to 50 mm is 0.46% (TM), 0.48% (QT). Higher limits apply to thicker plates.

What is the difference between CCS DH500 and the A, D, E and F grades of the same strength?

The strength requirements are identical; only the Charpy test temperature changes (0, −20, −40 or −60°C), and E/F grades have tighter P and S limits.

Equivalent steel grade of CCS/D500

DNV

GL

LR

BV

ABS

NK

KR

RINA

NV D500

GL-D500

LR/DH50

BV/D500

AB/DQ51

K D51

R D51

RI/D500

If you need more stock steel plates in shipbuilding steel plate, please click warehouse sizes.

Related steel grades: CCS/A500,CCS/D620, CCS/D550, CCS/E500

 

CCS Steel Plate Grade

General Strength

CCS/A

CCS/B

CCS/D

CCS/E

High Strength

CCS/A32

CCS/D32

CCS/E32

CCS/F32

CCS/A36

CCS/D36

CCS/E36

CCS/F36

CCS/A40

CCS/D40

CCS/E40

CCS/F40

Extra Strength

CCS/A420

CCS/D420

CCS/E420

CCS/F420

CCS/A460

CCS/D460

CCS/E460

CCS/F460

CCS/A500

CCS/D500

CCS/E500

CCS/F500

CCS/A550

CCS/D550

CCS/E550

CCS/F550

CCS/A620

CCS/D620

CCS/E620

CCS/F620

CCS/A690

CCS/D690

CCS/E690

CCS/F690

Other Products