RINA AH36 steel plate, also written as RI/AH36, RINA Grade AH36, Registro Italiano Navale AH36 or AH36 ship steel plate, is the higher-strength hull structural steel of RINA Rules for the Classification of Ships (IACS UR W11 higher-strength family) with 355 MPa minimum yield, 490-620 MPa tensile strength and Charpy V-notch toughness at 0°C [32°F]. In the grade name, "A" is the toughness class, "H" means higher strength and "36" refers to the strength level (historically about 36 kgf/mm²). Gangsteel, a steel plate exporter, supplies RINA AH36 / RI/AH36 plates cut to size for shipbuilding, offshore platforms and marine structures.

Data source: Per IACS UR W11 (ordinary/higher-strength hull structural steel) as adopted in RINA (Registro Italiano Navale) hull structural steel rules. Official mill/certificate grade is RINA AH36 (RI/AH36). Verify the current RINA edition before ordering.

RINA AH36 Chemical Composition (Heat Analysis)

 

ElementCMnSiPSAl (acid sol.)
RINA AH36, %0.18 max0.90-1.600.10-0.500.035 max0.035 max0.015 min
ElementNbVTiCuCrNi / Mo
RINA AH36, %0.02-0.050.05-0.100.02 max0.35 max0.20 max0.40 max / 0.08 max

Per IACS UR W11 / RINA hull structural steel rules (higher-strength grades). Nb, V and Al grain-refining elements may be used singly or in combination; when used in combination the individual minima do not apply. Where acid-soluble Al is not less than 0.015%, the Si minimum does not apply. Carbon equivalent: Ceq = C + Mn/6 + (Cr+Mo+V)/5 + (Ni+Cu)/15 (%).

Product Analysis (Check Analysis)

 

IACS UR W11 / RINA rules do not separately tabulate product (check) analysis limits for higher-strength grades. When product analysis is required, the finished plate shall meet the heat limits subject to ASTM A6/A6M Table A permitted variations (same practice as other IACS societies).

ElementHeat analysis limitProduct analysis (heat ± A6)
C0.18 max0.22 max
Mn0.90-1.600.81–1.72
Si0.10-0.500.04–0.56
P0.035 max0.045 max
S0.035 max0.045 max
Al (acid sol.)0.015 minno A6 Table A tolerance; product value not tabulated
Nb0.02-0.050.010–0.060
V0.05-0.100.040–0.110
Ti0.02 max0.03 max
Cu0.35 max0.38 max
Cr0.20 max0.24 max
Ni0.40 max0.43 max
Mo0.08 max0.09 max

Per IACS UR W11 / RINA hull structural steel rules. Product analysis applies only when specified; for a range, results may not vary both above and below it.

RINA AH36 Mechanical Properties

 

GradeYield strength, minTensile strengthElongation, min
RINA AH36355 MPa [51 ksi]490-620 MPa [71-90 ksi]21%

Per IACS UR W11 / RINA hull structural steel rules. Yield and tensile values apply for the full thickness range covered by the grade (typically up to 100 mm for these ship plates).

Charpy V-Notch Impact Requirements (0°C [32°F])

 

ThicknessTest temperatureLongitudinal, avg minTransverse, avg min
t≤50 mm0°C [32°F]34 J24 J
50<t≤70 mm0°C [32°F]41 J27 J
70<t≤100 mm0°C [32°F]50 J34 J

Per IACS UR W11 / RINA hull structural steel rules. Average of three full-size Charpy V-notch specimens; not more than one value below the average and none below 70% of it. Longitudinal values shown; transverse values apply when required by the rules or purchase order. Thicker plates (above 100 mm) may be supplied by agreement with adjusted impact requirements.

Delivery Condition and Deoxidation

Deoxidation: Killed, fine-grain practice. Delivery condition: A-class (AH36) grades may be as-rolled, controlled rolled, normalized or TMCP depending on thickness; thicker plates usually N or TMCP. Optional extras by agreement include ultrasonic testing, Z-direction (Z15/Z25/Z35) through-thickness testing and third-party RINA survey.

Thickness Coverage

Higher-strength RINA AH/DH/EH/FH 32/36/40 plates are commonly supplied from about 6 mm to 100 mm thick (up to 150 mm by agreement). Width 1500-4000 mm and length 6000-18000 mm are typical.

Equivalent Steel Grades of RINA AH36

 

Society / StandardEquivalent grade
RINA (Registro Italiano Navale)RINA AH36 steel plate (RI/AH36)
LR (Lloyd's Register)LR AH36 steel plate
ABSABS AH36 steel plate
CCSCCS AH36 steel plate
ASTM A131/A131MASTM A131 AH36 steel plate
GLGL AH36 steel plate
DNVDNV A36 steel plate
BVBV AH36 steel plate
NKNK A36 steel plate
KRKR A36 steel plate

IACS member societies harmonize ordinary and higher-strength hull grades under UR W11; dual certification (for example RINA + ABS, or RINA + ASTM A131) is common when ordered that way.

FAQ about RINA AH36 Steel Plate

What is RINA AH36 steel plate?

It is a higher-strength hull structural steel under RINA (Registro Italiano Navale) Rules for the Classification of Ships (IACS UR W11), with 355 MPa minimum yield, 490-620 MPa tensile strength and Charpy toughness at 0°C [32°F]. The mill certificate grade is RINA AH36 (RI/AH36).

What does RINA AH36 / RI/AH36 stand for?

RINA is Registro Italiano Navale (also abbreviated RI on mill certificates). The letter A is the toughness class (Charpy at 0°C [32°F]), H means higher strength, and 36 is the strength level (historically about 36 kgf/mm², now 355 MPa min yield).

What is the yield strength of RINA AH36?

Minimum 355 MPa (51 ksi), tensile 490-620 MPa (71-90 ksi), elongation about 21% min.

What is the impact test temperature for RINA AH36?

Charpy V-notch at 0°C [32°F]. Longitudinal average minima are 34 J up to 50 mm, 41 J for 50-70 mm and 50 J for 70-100 mm.

What is the difference between RINA AH36 and other 36-class grades?

Same 355 MPa strength class. RINA AH36 at 0°C [32°F]; RINA DH36 at -20°C [-4°F]; RINA EH36 at -40°C [-40°F]; RINA FH36 at -60°C [-76°F]. Delivery condition follows the toughness letter rules.

What is the difference between RINA AH36 and RINA AH32?

Same A-class toughness (Charpy at 0°C [32°F]). RINA AH36 is strength class 36 (355 MPa min yield); RINA AH32 is strength class 32 (315 MPa min yield).

Is RINA AH36 the same as ABS AH36 or LR AH36?

Requirements are essentially harmonized under IACS UR W11. ABS AH36, LR AH36, DNV A36, BV AH36, KR A36, NK A36 and ASTM A131 AH36 (where listed) are counterparts; dual certification is common when ordered with the required surveys.

Is RINA AH36 weldable?

Yes. Controlled carbon and Ceq give good weldability; preheat may be required for thick sections depending on Ceq and restraint.

What heat treatment is required for RINA AH36?

A-class (AH36) grades may be as-rolled, controlled rolled, normalized or TMCP depending on thickness; thicker plates usually N or TMCP.

What thickness is available for RINA AH36?

Typical supply is about 6-100 mm thick (up to 150 mm by agreement), 1500-4000 mm wide and 6000-18000 mm long.

Other RINA Steel Plate Grades

RINA Grade A steel plate | RINA Grade B steel plate | RINA Grade D steel plate | RINA Grade E steel plate | RINA AH32 steel plate | RINA AH40 steel plate | RINA DH32 steel plate | RINA DH36 steel plate | RINA DH40 steel plate | RINA EH32 steel plate | RINA EH36 steel plate | RINA EH40 steel plate | RINA FH32 steel plate | RINA FH36 steel plate | RINA FH40 steel plate

Equivalent Class Society Grades

RINA AH36 corresponds to the same grade under the other IACS member classification societies: LR AH36 steel plate, ABS AH36 steel plate, CCS AH36 steel plate, ASTM A131 AH36 steel plate, GL AH36 steel plate, DNV A36 steel plate, BV AH36 steel plate, NK A36 steel plate, KR A36 steel plate, RINA AH36 steel plate.

Other Products